聚氨酯防水涂料又名聚氨酯涂膜防水材料,是由含异氰酸酯基(-NCO)的聚氨酯预聚体(甲组分)和有多羟基(-NH2)的固定化剂及共助剂的混合物(乙组分)按一定比例混合形成的一种反应型涂膜防水材料。
该产品按组分分为单组分(S)多组分(M)两种;按拉伸性能分为I、II两类。
该产品可在潮湿或干燥的砖石、砂浆、混凝土、金属、木材硬塑料、玻璃、各种保温层、各种防水层上直接施工,适用于桥梁、高速公路、隧道水库等。
单组分聚氨酯性能指标
SN |
项目 Ltem |
I |
II |
|||
1 |
拉伸强度/MPa |
1.9 |
2.45 |
|||
2 |
断裂伸长率/% Elongation at breat/% ≥ |
550 |
450 |
|||
3 |
撕裂强度/(N/mm) Tear strength(N/mm) ≥ |
12 |
14 |
|||
4 |
低温弯折性/℃ Low temperature bend/℃ |
-40 |
||||
5 |
不透水性0.3MPa30min Waterproofness 0.3MPa30min |
不透水 Watertight |
||||
6 |
固体含量/% Solid content/% ≥ |
80 |
||||
7 |
表干时间/h Surface dry time/h |
12 |
||||
8 |
实干时间/h Solidity time/h |
24 |
||||
9 |
加热伸缩率/% Themal flexidle rete/% |
|
1.0 |
|||
≥ |
-4.0 |
|||||
10 |
潮湿基面粘结强度/aMPa Binding strength of wet underlying surface/MPa ≥ |
0.50 |
||||
11 |
定伸时老化 Aging of definite tensile elongation |
加热老化 Thermal aging |
No crack and distortion |
|||
人工气候老化b Artificial weathering agingb |
无裂纹及形变 No crack and distortion |
|||||
热处理 Heat treatment |
伸拉强度 Tensile strength |
80-150 |
||||
Elongation at break/% ≥ |
500 |
400 |
||||
Low temperature bend/℃ |
-35 |
|||||
13 |
碱处理 Alkali treatment |
60-150 |
||||
断裂伸长率/% Elongation at break/% ≥ |
500 |
400 |
||||
低温弯折性/℃ Low temperature bend/℃ |
-35 |
|||||
14 |
酸处理 Alkaline treatment |
拉伸强度保持率/% Holding of tensile strength/% |
80-150 |
|||
Elongation at break/% ≥ |
500 |
400 |
||||
低温弯折性/℃ Low temperature bend/℃ |
-35 |
|||||
15 |
人工气候老化 Acid treatment |
拉伸强度保持率/% Holding of tensile strength/% |
80-150 |
|||
断裂伸长率/% Elongation at break/% ≥ |
500 |
400 |
||||
低温弯折性/℃ Low temperature bend/℃ |
-35 |
|||||
a仅用于地下工程 潮湿基面的要求。 b仅用于外露使用的产品。 a Only used for the wet underlying surface under the ground. b Only used for the for the products of exposed application. |
双组份聚氨酯防水涂料性能指标
序号 SN |
项目 Ltem |
I |
II |
||
1 |
拉伸强度/MPa Tenslile stength/Mpa ≥ |
1.9 |
2.45 |
||
2 |
断裂伸长率/% Elongation at breat/% ≥ |
450 |
450 |
||
3 |
撕裂强度/(N/mm) Tear strength(N/mm) ≥ |
12 |
14 |
||
4 |
低温弯折性/℃ Low temperature bend/℃ ≤ |
-35 |
|||
5 |
不透水性0.3MPa30min Waterproofness 0.3MPa30min |
不透水 Watertight |
|||
6 |
固体含量/% Solid content/% ≥ |
92 |
|
||
7 |
表干时间/h Surface dry time/h ≤ |
8 |
|
||
8 |
实干时间/h Solidity time/h ≤ |
24 |
|
||
9 |
加热伸缩率/% Themal flexidle rete/% |
≤ |
1.0 |
||
≥ |
-4.0 |
||||
10 |
潮湿基面粘结强度/aMPa Binding strength of wet underlying surface/MPa ≥ |
0.50 |
|||
11 |
定伸时老化 Aging of definite tensile elongation |
加热老化 Thermal aging |
无裂纹及形变 No crack and distortion |
||
人工气候老化b Artificial weathering agingb |
无裂纹及形变 No crack and distortion |
||||
12 |
热处理 Heat treatment |
伸拉强度 Tensile strength |
80-150 |
||
断裂伸长率/% Elongation at break/% ≥ |
400 |
||||
低温弯折性/℃ Low temperature bend/℃ ≤ |
-30 |
||||
13 |
碱处理 Alkali treatment |
拉伸强度保持率/% Holding of tensile strength/% |
60-150 |
||
断裂伸长率/% Elongation at break/% ≥ |
400 |
||||
低温弯折性/℃ Low temperature bend/℃ ≤ |
-30 |
||||
14 |
酸处理 Alkaline treatment |
拉伸强度保持率/% Holding of tensile strength/% |
80-150 |
||
断裂伸长率/% Elongation at break/% ≥ |
400 |
||||
低温弯折性/℃ Low temperature bend/℃ |
-35 |
||||
|
|
拉伸强度保持率/% Holding of tensile strength/% |
80-150 |
||
断裂伸长率/% Elongation at break/% |
400 |
||||
低温弯折性/℃ Low temperature bend/℃ |
-30 |
||||
a仅用于地下工程 潮湿基面的要求。 b仅用于外露使用的产品。 a Only used for the wet underlying surface under the ground. b Only used for the for the products of exposed application. |
● 基层要求
1.基层表面应压实平整,采用水泥砂浆找平时,必须充分养护,不得有酥松、起砂、起皮现象、应符合设计要求。
2.混凝土表面要进行拉毛、刨铣或抛丸处理。
3.桥面含水率不应大于15%。
● 施工操作
1.基层清理完毕以后,应将阴阳角、伸缩缝、施工缝等重点部位进行处理。
2.重点部位处理完毕应按施工要求,配比涂刷底子油,以提高粘合强度和抗剪切强度。
3.底子油干后可涂刷或喷涂防水涂料。
4.防水层要符合设计标准规范。并可根据设计要求增设纤维等增强层。在摊铺沥青前可采取在防水层表面撒布细粒沥青混合料的方法做成隔离层,以防涂膜受损。